Home > Knowledge > Content

How to repair the hydraulic cylinder piston rod?

Feb 25, 2024

After the piston rod of the gas-liquid boosting cylinder is strained during work, if it is not dealt with in time, it will affect the use of the product at least, and in serious cases, the hydraulic cylinder will not work. So how do we fix it?
Lighter scratches will be repaired by local grinding and polishing; heavier scratches will be repaired by welding and manual grinding.
Formation of pull marks: After the gas-liquid boosting cylinder was disassembled, it was found that one of the piston rods of the luffing cylinder was severely strained, with 6 pull marks side by side.
The main reason for the piston rod strain is that after the dust ring becomes brittle and falls off in a block, it not only loses its dustproof effect, but also accumulates a lot of dust and magazines on the expansion joint, causing the piston rod to grind directly against impurities, causing the piston to become damaged. The rod was stretched, and the scratches scratched the rubber sealing component of the cylinder mouth, causing serious leakage of the hydraulic cylinder.
Repair requirements: The filler and base material must be firmly and smoothly combined; the seasoning must be durable and easy to process by hand; manual processing must ensure that the piston rod diameter error is less than 0.06mm.
After analysis, it was decided that the filler used was J422 electrode. Because acidic welding rods are insensitive to rust, oil and moisture, and are not prone to hydrogenation holes; they have good craftsmanship and are easy to operate; the welds are beautifully formed; the material has moderate hardness and is easy to be processed by hand; the arc is stable, the penetration is large, and it is consistent with the base material The bond is strong.
Repair process:
(1) Clean the area to be welded first, and then surround the pull marks with wet mud.
(2) Use a welding rod with a diameter of 2.5mm, adjust the current of the welding machine to 120A, and use the straight-line rod movement method to perform welding smoothly.
(3) After all welding is completed, clean away the mud and slag, use a rough rasp to file along the circumference of the piston rod and leave a machining allowance of 0.1-0.2mm.
(4) Use a cylinder with an outer diameter of 185mm, an inner diameter of 125mm, and a length of 150mm as a master (the outer diameter of the piston rod is 125mm), and saw it along the axis. One is a rough mold and the other is a fine mold.
(5) Apply a thin layer of red stamp oil on the inner wall of the rough mold, then place the rough mold against the part to be repaired on the piston rod and run it back and forth along the axis several times, and then use a fine file to remove the heavier red stamp on the piston rod. File it off. Repeat the filing process in this way until a machining allowance of 0.04-0.07mm is left.
(6) Then use a 320-mesh sand bar dipped in kerosene and match the precision mold to grind the piston rod to the specified size.
(7) Finally, use the back of the emery cloth dipped in kerosene for manual polishing. After measurement, the maximum error is only 0.03mm.
After the repair of the gas-liquid boosting cylinder, after one and a half years of use, the luffing hydraulic cylinder has never leaked. At the same time, the piston rod is smooth and has no rust spots.